TOP 35 Corrosion Resistant Alloys Group
| ★ = Good to excellent ✩ = Acceptable – = Not suitable | ||||||||
|---|---|---|---|---|---|---|---|---|
| Phosphoric Acid | Hydrochloric Acid | Sulfuric Acid | Hydrofluoric Acid | Organic Acid | Nitric Acid | Seawater | Alkalines & Salts | |
| Alloy 201 | ✩ | ✩ | ✩ | ★ | ★ | – | ✩ | ★ |
| Alloy 200 | ✩ | ✩ | ✩ | ★ | ★ | – | ✩ | ★ |
| DURANICKEL® Alloy 301 | ✩ | ✩ | ✩ | ★ | ★ | – | ✩ | ★ |
| Alloy R-405 | ★ | ✩ | ★ | ★ | ★ | – | ★ | ★ |
| Alloy 400 | ★ | ✩ | ★ | ★ | ★ | – | ★ | ★ |
| Alloy K-500 | ★ | ✩ | ★ | ★ | ★ | – | ★ | ★ |
| Alloy 622 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 600 | ✩ | – | ✩ | ✩ | ★ | – | ✩ | ★ |
| Alloy 625 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 686 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 625LCF® | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 718 | ✩ | ✩ | ✩ | ✩ | ★ | ✩ | ★ | ★ |
| Alloy 690 | ★ | ✩ | ✩ | ★ | ★ | ★ | ✩ | ★ |
| Alloy 725™ | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy G-3 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy C-276 | ★ | ★ | ★ | ★ | ★ | ✩ | ★ | ★ |
| Alloy 800 | ✩ | ✩ | ✩ | – | ★ | ★ | ✩ | ✩ |
| Alloy 25-6MO | ★ | ★ | ★ | ✩ | ★ | ★ | ★ | ★ |
| Alloy 050 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 825 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 925™ | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 864™ | ✩ | ✩ | ✩ | ✩ | ★ | ★ | ★ | ★ |
| Alloy 020 | ★ | ★ | ★ | ★ | ★ | ★ | ★ | ★ |
| Alloy 028 | ✩ | ★ | ✩ | ✩ | ★ | ★ | ★ | ★ |
Corrosion Resistant Steel Features
| Classification | Alloy | Features |
|---|---|---|
| Corrosion Resistant Alloys | Alloy 400 |
|
| Alloy 201 | Good cold workability, | |
| Alloy K-500 |
|
|
| Alloy 200 |
|
|
| Alloy 600 |
|
|
| Alloy 760 |
|
|
| Alloy 625 |
|
|
| Alloy C-276 |
|
|
| Alloy 22 |
|
|
| Alloy CB3 |
|
|
| Alloy 25-6MO |
|
What Makes a Material Corrosion-Resistant?
Application Of Corrosion Resistant Material
| Classification | Alloy | Applications |
|---|---|---|
| Corrosion Resistant Alloys | Alloy 400 |
|
| Alloy 201 | Cold deep-drawn parts | |
| Alloy K-500 |
|
|
| Alloy 200 |
|
|
| Alloy 600 |
|
|
| Alloy 760 |
|
|
| Alloy 25-6MO |
|
|
| Alloy 22 |
|
|
| Alloy 625 |
|
|
| Alloy C-276 |
|
Corrosion Resistant Steel Grades Chemical Composition
| Nominal Chemical Compositions (% by weight) | ||||||||
|---|---|---|---|---|---|---|---|---|
| Designation | Werkstoff | UNS | Cr | Ni | Fe | Mo | Other | Cu |
| Nickel 201 | 2.4061 | N02201 | 99.6 | C 0.02 max. | ||||
| Nickel 200 | 2.4060 | N02200 | 99.6 | C 0.04 | ||||
| Alloy 400 | 2.4360 | N04400 | 65.1 | 1.6 | Mn 1.1 | 32.0 | ||
| Alloy 600 | 2.4816 | N06600 | 15.0 | 76.0 | 8.0 | |||
| Alloy K-500 | 2.4375 | N05500 | 64.7 | 1.0 | Al 2.7, Ti 0.6 | 30.2 | ||
| Alloy 622 | 2.4602 | N06022 | 20.5 | 59.0 | 2.3 | 14.2 | W 3.2 | |
| Alloy 686 | 2.4606 | N06686 | 20.5 | 58.0 | <1.0 | 16.3 | W 3.8 | |
| Alloys 625 and 625LCF | 2.4856 | N06625 N06626 | 21.5 | 61.0 | 2.5 | 9.0 | Nb 3.6 | |
| Alloy 690 | 2.4642 | N06690 | 29.0 | 61.5 | 9.0 | |||
| Alloy 725 | N07725 | 21.0 | 57.0 | 7.5 | 8.0 | Nb 3.5, Ti 1.5, Al 0.3 | ||
| Alloy 718 | 2.4668 | N07718 | 18.0 | 54.0 | 18.5 | 3.0 | Nb 5.0, Ti 1.0 | |
| Alloy C-276 | 2.4819 | N10276 | 16.0 | 57.0 | 5.5 | 16.0 | W 4.0 | |
| Alloy 050 | N06950 | 20.0 | 50.0 | 17.0 | 9.0 | |||
| Alloy G-3 | 2.4619 | N06985 | 22.0 | 44.0 | 19.5 | 7.0 | 2.0 | |
| Alloy 800 | 1.4876 | N08800 | 21.0 | 32.5 | 46.0 | C 0.05 | ||
| Alloy 864 | S35135 | 21.0 | 34.0 | 39.0 | 4.2 | Si 0.8, Ti 0.6 | ||
| Alloy 825 | 2.4858 | N08825 | 21.5 | 42.0 | 28.0 | 3.0 | 2.0 | |
| Alloy 925 | N09925 | 21.0 | 44.0 | 28.0 | 3.0 | Ti 2.1, Al 0.3 | 1.8 | |
| Alloy 028 | 1.4563 | N08028 | 27.0 | 32.0 | 3.5 | Mn 2.0 | 1.0 | |
| Alloy 020 | 2.4660 | N08020 | 20.0 | 35.0 | 37.0 | 2.5 | Nb 0.6 | 3.5 |
| Alloy 25-6MO | 1.4529 | N08926 | 20.0 | 25.0 | 47.0 | 6.5 | N 0.20 | 0.9 |
Austenitic Stainless Steel
| Grade | EN Specification | Phosphorus (P) | Nickel (Ni) | Manganese (Mn) | Chromium (Cr) | Iron (Fe) | Silicon (S) | Carbon (C) | Molybdenum (Mo) | Sulfur (S) | Nitrogen (N) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| 301 | 1.4310 | 0.045 | 6.0 – 9.5 | 2.00 | 16.0 – 19.0 | Balance | 2.00 | 0.05 – 0.15 | 0.80 | 0.015 | 0.10 |
| 304 | 1.4301 | 0.045 | 8.0 – 10.5 | 2.00 | 17.5 – 19.5 | Balance | 1.00 | 0.07 | – | 0.015 | 0.1 |
| 304L | 1.4307 | 0.045 | 8.0 – 10.5 | 2.00 | 17.5 – 19.5 | Balance | 1.00 | 0.03 | – | 0.015 | 0.1 |
| 201 | 1.4372 | 0.045 | 3.5 – 5.5 | 5.5 – 7.5 | 16.0 – 18.0 | Balance | 1.00 | 0.15 | – | 0.015 | 0.05 – 0.25 |
| 316 | 1.4401 | 0.045 | 10.0 – 13.0 | 2.00 | 16.5 – 18.5 | Balance | 1.00 | 0.07 | 2.0 – 2.5 | 0.015 | 0.1 |
| 316L | 1.4404 | 0.045 | 10.0 – 13.0 | 2.00 | 16.5 – 18.5 | Balance | 1.00 | 0.03 | 2.0 – 2.5 | 0.015 | 0.1 |
Ferritic Stainless steel
| EN Specification | Grade | Sulfur (S) |
Carbon (C) |
Phosphorus (P) |
Silicon (Si) |
Manganese (Mn) |
Chromium (Cr) |
Titanium (Ti) |
Nickel (Ni) | Molybdenum (Mo) |
Niobium (Nb) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| 1.4513 | 436 | 0.015 | 0.025 | 0.040 | 1.00 | 1.00 | 16.0 – 18.0 | [4 x (C + N) + 0.15] to max 0.8 | 0.020 | 0.80 – 1.40 | – |
| 1.4016 | 430 | 0.015 | 0.080 | 0.040 | 1.00 | 1.00 | 16.0 – 18.0 | – | – | – | – |
| 1.4512 | 409 | 0.015 | 0.030 | 0.040 | 1.00 | 1.00 | 10.5 – 12.5 | [6 x (C + N)] to max 0.65 | – | – | – |
| 1.4113 | 434 | 0.015 | 0.080 | 0.040 | 1.00 | 1.00 | 16.0 – 18.0 | – | – | – | – |
| 1.4510 | 439 | 0.015 | 0.050 | 0.040 | 1.00 | 1.00 | 16.0 – 18.0 | [4 x (C + N) + 0.15] to max 0.8 | – | – | (3 x C + 0.3) to max 1 |
| 1.4509 | 4509 | 0.015 | 0.030 | 0.040 | 1.00 | 1.00 | 17.5 – 18.5 | 0.1 – 0.6 | – | – | – |
Martensitic Stainless Steel
| EN Specification | Grade | Carbon (C) | Iron (Fe) | Silicon (S) | Manganese (Mn) | Phosphorus (P) | Sulfur (S) | Chromium (Cr) | Nickel (Ni) | Nitrogen (N) |
|---|---|---|---|---|---|---|---|---|---|---|
| 1.4006 | 410 | 0.08 – 0.15 | Balance | 1.00 | 1.50 | 0.040 | 0.015 | 11.5 – 13.5 | 0.75 | – |
| 1.4021 | 420 | 0.16 – 0.25 | Balance | 1.00 | 1.50 | 0.040 | 0.015 | 12.0 – 14.0 | – | – |
| 1.4031 | 420 | 0.07 | Balance | 1.00 | 2.00 | 0.045 | 0.015 | 17.5 – 19.5 | 8.0 – 10.5 | 0.1 |
Physical Properties Of Corrosion Resistant Alloys
| Alloy | Density | Mechanical Properties at Nominal Room-temperature | ||||||
|---|---|---|---|---|---|---|---|---|
| Tensile strength | 0.2% yield strength | Hardness | Elongation | |||||
| lb/in3 | g/cm3 | ksi | MPa | ksi | MPa | Brinel | % | |
| Alloy 201 | 0.321 | 8.89 | 60 | 414 | 35 | 241 | 100 | 50 |
| Alloy 200 | 0.321 | 8.89 | 65 | 448 | 30 | 207 | 110 | 45 |
| MONEL® Alloy 400 | 0.318 | 8.80 | 80 | 552 | 40 | 276 | 140 | 45 |
| DURANICKEL® Alloy 301 (aged) | 0.296 | 8.19 | 160 | 1100 | 125 | 860 | 340 | 25 |
| MONEL® Alloy K-500 (aged) | 0.305 | 8.44 | 155 | 1069 | 100 | 689 | 310 | 25 |
| MONEL® Alloy R-405 (stress-relieved) | 0.318 | 8.80 | 95 | 655 | 85 | 586 | 205 | 25 |
| Alloy 600 | 0.306 | 8.47 | 100 | 689 | 50 | 345 | 170 | 40 |
| Alloy 625 | 0.305 | 8.44 | 125 | 862 | 65 | 448 | 200 | 50 |
| Alloy 622 | 0.311 | 8.61 | 115 | 793 | 55 | 379 | 170 | 60 |
| Alloy 625LCF® | 0.305 | 8.44 | 130 | 896 | 70 | 483 | 255 | 50 |
| Alloy 690 | 0.296 | 8.19 | 100 | 689 | 50 | 345 | 170 | 45 |
| Alloy 686 | 0.315 | 8.73 | 110 | 758 | 55 | 379 | 180 | 60 |
| Alloy 725™ (aged) | 0.300 | 8.30 | 185 | 1276 | 130 | 896 | 355 | 30 |
| Alloy 718 (aged) | 0.296 | 8.19 | 205 | 1413 | 165 | 1138 | 425 | 20 |
| Alloy G-3 | 0.294 | 8.14 | 105 | 724 | 55 | 379 | 140 | 40 |
| Alloy C-276 | 0.321 | 8.89 | 110 | 758 | 50 | 345 | 180 | 60 |
| Alloy 800 | 0.287 | 7.94 | 90 | 621 | 50 | 345 | 165 | 40 |
| Alloy 050 (as drawn) | 0.303 | 8.39 | 130 | 896 | 125 | 862 | 326 | 13 |
| Alloy 825 | 0.294 | 8.14 | 95 | 655 | 45 | 310 | 155 | 45 |
| Alloy 925™ (aged) | 0.292 | 8.08 | 170 | 1172 | 120 | 827 | 320 | 25 |
| Alloy 864™ | 0.290 | 8.02 | 95 | 655 | 40 | 276 | 150 | 45 |
| Alloy 25-6MO | 0.290 | 8.03 | 110 | 758 | 55 | 379 | 180 | 45 |
| Alloy 020 | 0.292 | 8.08 | 95 | 655 | 60 | 414 | 180 | 35 |
| Alloy 028 | 0.290 | 8.03 | 90 | 621 | 40 | 276 | 160 | 40 |
Stainless Steel
| Condition | Steel & Alloy Material Type | Ultimate Tensile Strength (PSI) | 0.2% Yield Strength (PSI) | Elongation (% In 2in.) | Reduction Of Area (%) | Hardness Brinell | Hardness Rockwell |
|---|---|---|---|---|---|---|---|
| Annealed | 304 | 75,000 | 30,000 | 30 | 40 | * | * |
| Annealed | 304L | 70,000 | 25,000 | 30 | 40 | * | * |
| Annealed | 317 | 75,000 | 30,000 | 30 | 40 | * | * |
| Annealed | 316 | 75,000 | 30,000 | 30 | 40 | * | * |
| Annealed | 316L | 70,000 | 25,000 | 30 | 40 | * | * |
| H950 | PH 13-8 | 220,000 | 205,000 | 10 | 35 | 430 | C45 |
| Annealed | 317L | 70,000 | 25,000 | 30 | 50 | * | * |
| T | 410 | 100,000 | 80,000 | 12 | 40 | * | * |
| Annealed | 70,000 | 40,000 | 16 | 45 | * | * | |
| Tempered | * | * | * | * | 248-302 | * | |
| NACE MRO 175 | * | * | * | * | * | 22 HRC Max | |
| H | 120,000 | 90,000 | 12 | 40 | * | * | |
| Annealed | 416 | * | * | * | * | 262 Max | * |
| Class2 | 110,000 | 85,000 | 15 | 45 | 269 Max | * | |
| Hardened | * | * | * | * | 293-352 | * |
Point to Consider Selecting the Right Corrosion Resistant Material
Welding Corrosion Resistant Alloys
| Common Welding Method Used | Factor to Consider At Time Of Welding | Welding Challenges |
|---|---|---|
|
|
|
Corrosion Tests Of Corrosion Resistant Metal
| In Impure 12% Hydrofluoric Acid Plant Corrosion Tests | |
|---|---|
| Material | Corrosion rate, mpy (mm/a) |
| MONEL alloy 400 | 22 (0.30) |
| Nickel 200 | 4 (0.10) |
| INCONEL alloy 600 | 9 (0.23) |
| AISI 302 stainless steel | 160 (4.06)b |
| AISI 316 stainless steel | 700 (17.8)b |
| in the Storage of Commercial 60-65% Hydrofluoric Acid Plant Corrosion Tests | |
|---|---|
| Material | Corrosion rate, mpy (mm/a) |
| Mild Steel | 170 (4.32) |
| Nickel 200 | >200 (>5.08)b |
| MONEL alloy 400 | 22 (0.56) |
| AISI 304 stainless steel | >210 (>5.33)b |
| INCONEL alloy 600 | 150 (3.81) |
| AISI 316 stainless steel | >190 (>4.83)b |
| Nickel Alloys Corrosion-resistance in 24-hour Tests in Boiling Acetic Acid | |||
|---|---|---|---|
| Alloy | Acetic acid concentration | Corrosion rate | |
| mm/a | mpy | ||
| INCONEL alloy 686 | 80% | <0.01* | <0.1* |
| INCONEL alloy 625 | 10% | 0.01-0.019 | 0.39-0.77 |
| INCOLOY alloy 825 | 10% | 0.0152-0.0160 | 0.60-0.63 |
| INCONEL alloy C-276 | 10% | 0.011-0.0114 | 0.41-0.45 |
Difference Between Corrosion and Rust
| Factor | Corrosion | Rust |
|---|---|---|
| Appear On | All alloys and metals | Just Iron and Its Alloys in |
| Reason | Oxygen, Moisture, Salt, Chemicals, Acids | Oxygen and Moisture |
| Color | Different ( green, white, gray, etc.) | Brownish-Red Flakes |
| Speed | Varies with metal and environment type | Faster in salty and humid conditions |
| Prevention | cathodic protection,Coatings, alloying, inhibitors | rust-resistant paints |
Additional service : Small quantity | Custom order | hard to find items | Sourcing from other countries
Why Siddhagiri Metals & Tubes ?
Table of Content